Pollutant Guides By Dr. Maximilian Mandl 26 min read

When is a coating lead paint? The threshold values compared

0.35 percent lead in an old coating, is that a lot? Why that number does not define lead paint, which limits really apply, and what the intermediate range means. Every value with a source.

Suppose a laboratory reports 3,500 mg/kg of lead for an old door coating, that is 0.35 percent by mass. Is that a lot? Is it now a "lead paint" that must be remediated? The value sits in an awkward middle: almost forty times the maximum that the United States and the UN Environment Programme's model law set for new paint, yet one to two orders of magnitude below a classic lead-white coating. Not nothing, but not an obvious lead paint either. What is it, and why is there lead in it at all?

It is precisely this intermediate range, roughly between one tenth and a full percent by mass, where most of the confusion arises. Above about one percent everyone agrees, below about one hundredth of a percent too. In between, the yardsticks collide. This page first explains why an old coating lands in this range, then places the value against every yardstick that actually exists, and shows how lead content is properly measured. Every value is sourced, almost every one at the primary source; where the primary source is not freely accessible, the text says so. This post is a factual reference, not legal advice. The three numbers used here as examples (0.2, 0.35 and 0.7 percent by mass) are constructed, typical values, not an actual measurement.

Why an old coating lands in the intermediate range

A classic covering lead-white coating contains double-digit percentages of lead; the German TRGS 505 gives contents of lead and lead compounds of up to several hundred grams per kilogram of paint for covering paint coats and rust-protection coats (TRGS 505, Annex 3). A value of a few tenths of a percent arises by other routes. Three are typical, and they explain why "a little lead" is not the same as "lead paint".

Lead as a drier (siccative). Oil and alkyd paints harden through oxidative cross-linking, and this process is catalysed by metal soaps, the so-called driers. Lead was one of the classic drier metals, alongside cobalt, manganese and others (Paint & Coatings Industry 2011). As a lead soap, for example lead naphthenate or lead octoate, it is added only at a fraction of a percent of metal relative to the binder; typical metal contents of driers lie in the range of a few tenths of a percent (US Patent 4,631,087). Crucially, a drier is not a pigment. A coating can therefore contain lead from the drier without ever having seen a white lead pigment.

Lead as a minor constituent of a pigment. Not every lead pigment is the dominant white. Red lead (lead tetroxide, Pb3O4, elemental lead fraction around 90 percent) served as a rust-protective primer directly on iron and steel (IARC 2006); beneath several later top coats its lead becomes a minority share of the overall sample. Lead chromate (PbCrO4, lead fraction around 64 percent) was, as chrome yellow, a yellow pigment (IARC 2006). Lead white itself (mostly basic lead carbonate, lead fraction around 80 percent) was the most important white pigment until the end of the nineteenth century (ColourLex).

The layer effect. A laboratory sample that captures several layers together averages across all of them. A thin, highly leaded layer beneath several lead-free top coats vanishes in the mean: the bulk value can sit at a third of a percent even though a single layer beneath it carries a multiple of that. A mid-range mass percentage can therefore mean two things, "slightly leaded throughout" or "one critical old layer under clean new ones", and the two look identical in the laboratory average (HUD 2012).

For experts (or the expert-curious): elemental lead versus lead compound

A laboratory measures total elemental lead via digestion of the sample. For classification under CLP (see below) this is also the relevant quantity: the group entry "lead compounds with the exception of those specified elsewhere in this Annex" (index 082-001-00-6) and the individual entries such as lead chromate (082-004-00-2) carry Note 1 on the classification of mixtures in Annex VI (Annex VI Part 1, section 1.1.3.2). Under it, the concentration limits "are the percentages by weight of the metallic element calculated with reference to the total weight of the mixture". An elemental laboratory value can therefore be held directly against the 0.3 percent limit.

Austrian waste law also knows the calculation via the compound. The Waste Catalogue Ordinance requires a measured result to be converted to the most probable compound ("auf die am wahrscheinlichsten zutreffende Verbindung umzurechnen", Annex 4), and a lead compound weighs more than its lead: lead white contains around 80 percent lead, lead chromate around 64 percent, red lead around 90 percent (molar-mass calculation from the respective formulae). An elemental value of 0.2 percent corresponds, were the lead present as lead chromate, to around 0.31 percent compound. The same annex at the same time allows the CLP notes on the classification of mixtures, Note 1 among them, to be taken into account "gegebenenfalls" (where appropriate).

The most common misconception: 0.3 percent is not a lead-paint definition

The 0.3 percent that keeps coming up in connection with lead coatings is not a threshold above which a coating is called "lead paint". It comes from chemicals law: it is the generic concentration limit at which a mixture must be classified as reproductive toxicant category 1A or 1B (CLP Regulation, Annex I, Table 3.7.2; for category 2 it is 3.0 percent). That is a classification and labelling rule for mixtures, not a statement about an old coating on a wall.

More clearly still: in Austria and in Germany there is no legally binding threshold at all above which an old coating counts generally as "lead paint" or as requiring remediation. For old coatings, regulation works not through a coating-specific percentage but through three quite different quantities: the material content (percent by mass), the air at the workplace (milligrams per cubic metre) and the blood of the person working (micrograms per decilitre). These three cannot be converted into one another, and that is where most of the confusion comes from.

For experts (or the expert-curious): why there are two lead values (0.3 and 0.03 percent)

Lead is classified EU-wide, in harmonised form, as reproductive toxicant category 1A, and appears in Annex VI of the CLP Regulation with two separate entries, distinguished by particle size (introduced by an adaptation to technical and scientific progress, Regulation (EU) 2016/1179, applicable since 1 March 2018).

Lead powder (particle diameter below 1 mm, index 082-013-00-1) carries a specific concentration limit of 0.03 percent for the developmental effect (H360D). Lead massive (particle diameter from 1 mm, index 082-014-00-7) carries no specific limit of its own; here the generic value of 0.3 percent applies. The regulation's recital names both side by side.

What matters is the reach of these values. The two entries concern metallic lead. For a paint, that is a mixture with lead compounds such as lead carbonate or lead chromate, the generic value of 0.3 percent applies to damage to the unborn child (H360D), calculated as lead (Note 1, see the foldout above); neither the group entry for lead compounds (082-001-00-6) nor the entry for lead chromate (082-004-00-2) sets a specific limit for it. The 0.03 percent of the lead-powder entry describes metallic lead powder, not the compound dust produced when a coating is sanded. A 0.03 percent threshold for powdery lead-containing mixtures is set by the German TRGS 505 (see occupational safety); whether the sanding dust of a coating falls under it, the TRGS does not say expressly. The number 0.03 percent thus exists in both worlds, for related but not identical reasons.

Product law for new paints: the 90-ppm contrast

For paints sold today, a lead ban applies in practice in the United States: the consumer product authority CPSC declares consumer paint with more than 90 ppm (0.009 percent by mass) of lead, calculated as metal and based on the dried paint film, a banned hazardous product since 14 August 2009 (16 CFR 1303.1). The model law for regulating lead paint, developed by the UN Environment Programme UNEP together with the WHO and the US environmental agency EPA, proposes the same value, 90 ppm total lead, because it is the lowest existing legal limit. Canada likewise limits consumer paint to 90 mg/kg of total lead, Switzerland prohibits placing paints on the market from a lead content of 0.01 percent. The classification matters: 90 ppm is an international model and product benchmark, not an EU or Austrian value. In Austria and the EU there is no separate limit on the lead content of new paint of the kind the United States has. Instead, the classic lead pigments lead carbonate (lead white) and lead sulphate are banned specifically as paint constituents, in Austria by the Chemicals Prohibition Ordinance 2003 (section 11d), EU-wide by the REACH Regulation (Annex XVII, entries 16 and 17); the Austrian ordinance exempts the restoration of works of art and historic buildings, the REACH Regulation allows Member States such an exemption. In addition, mixtures containing lead compounds from the general classification limit of 0.3 percent, or lead powder from 0.03 percent, may not be supplied to the general public, with artists' paints among the exceptions (REACH Annex XVII, entry 30 with Appendix 5).

Worldwide, even this product law is not yet a given: as of 31 March 2023, according to the WHO and UNEP, only 93 countries had legally binding limits for lead in paint, with 19 more in the final stages of legislation.

For an old coating this yardstick is only a contrast, not a measure of assessment. A historic lead-white coating, with its double-digit percentages, lies more than a thousand times above 90 ppm. Even the constructed example value of 0.35 percent lies almost forty times above it. The real question with existing coatings is a different one.

Existing coatings: mass- and area-based definitions, and their absence here

Anyone seeking a robust definition of "lead-containing old coating" will not find one everywhere, but in some countries. Best known is the US definition: the environmental agency EPA (40 CFR 745.103) and the housing agency HUD (24 CFR 35.86) define "lead-based paint" word for word as a coating with at least 1.0 milligram of lead per square centimetre (area-based, usually measured with an X-ray device) or at least 0.5 percent by mass (5,000 mg/kg) of total lead. The "or" matters, and so does the "at least": both criteria are lower bounds, a coating can already be "lead-based paint" via the area criterion even though it is below 0.5 percent by mass.

Other countries draw the line elsewhere. France, for the "constat de risque d'exposition au plomb" (CREP), which is mandatory on the sale or letting of dwellings built before 1949, sets the threshold for lead-containing coatings at 1 milligram of lead per square centimetre, measured with a portable X-ray fluorescence device; if a laboratory analysis is also carried out, 1.5 mg/g of acid-soluble lead applies regardless of the X-ray result (Arrêté of 19 August 2011, Article 5). Australia, with the 2017 revision, lowered the concentration from which its management standard AS/NZS 4361.2 applies from 1 percent to 0.1 percent by mass (according to a technical bulletin of Environmental Health Australia, South Australia; the standard text itself is not freely available).

The key point: none of these actual existing-coating definitions sits at 0.3 percent. The United States set theirs at 0.5 percent by mass, Australia at 0.1 percent, France at 1 mg/cm² or, in the laboratory, at 1.5 mg/g of acid-soluble lead, that is 0.15 percent. And in Austria as in Germany there is no building-related "lead paint" threshold at all. A targeted search of the relevant bodies of law (limit-value ordinance, health surveillance, chemicals and waste law; in Germany the hazardous-substances rules and the TRGS) finds no such value; a complete negative proof across the entire legal order cannot be produced, but the relevant regulations contain none. The blanket equation "over 0.3 percent, therefore lead paint" is thus doubly wrong: 0.3 percent is, first, a classification limit and not a lead-paint definition, and it coincides, second, with not a single one of the existing-coating definitions that actually exist.

How lead content is measured

That the US definition has two criteria, one area-based and one mass-based, is no accident but reflects two quite different measurement methods.

The X-ray fluorescence device (XRF) measures the area loading on site, that is the mass of lead per area in milligrams per square centimetre. This quantity does not depend on how many lead-free top coats lie above it (HUD 2012). The radiation does, however, have to come back out of the depth: according to HUD, the K X-rays of lead penetrate many layers of paint, while L X-rays from deeper layers are less likely to reach the surface, so that instruments evaluating L X-rays alone detect lead in deep layers with more difficulty. XRF measures quickly and usually without damaging the coating, but says nothing about the percentage content of an individual layer.

Laboratory analysis takes the opposite route: from a removed material sample the lead content is determined as a mass fraction, in percent or in milligrams per kilogram (0.5 percent by mass corresponds to 5,000 mg/kg). Evaluated layer by layer, it resolves exactly the ambiguity that a bulk sample creates: it shows whether the lead is thinly distributed everywhere or sits in a single old layer.

The two quantities measure different things and cannot be converted into one another. This is not carelessness but physics: additional lead-free top coats lower the mass fraction in percent but do not change the area loading (HUD 2012). Anyone wanting to know the lead content of a particular coating therefore cannot avoid a professional investigation; it cannot be judged with the naked eye.

For experts (or the expert-curious): why mg/cm² and percent cannot be converted

The area concentration (mg/cm²) is a mass of lead per area and is independent of the thickness of the layer stack. The mass fraction (percent) is a mass of lead per total mass of the sample. The only thing mediating between them is the area weight of the layer, that is mass per area, and that is normally unknown. The HUD guideline puts it unambiguously: one cannot convert percent or ppm into an area concentration unless the total mass per unit area of the sample is known, because adding further lead-free layers changes the mass fraction but not the area concentration (HUD 2012).

As a rough rule of thumb for multi-layer old-building coatings, the same source states in its appendix that 1 mg/cm² corresponds on average to about 1 percent lead. That is expressly a statistical average across typical layer stacks, not a reliable conversion formula for the individual case.

Waste: when lead-containing material becomes hazardous

On removal the question of disposal arises. In Austria, Annex 3 of the Waste Catalogue Ordinance 2020 determines when a waste is hazardous, and for lead-containing material several hazard-relevant properties come into question there. The reproductive-toxicity property HP 10 is met if the waste contains 0.3 percent by mass or more of a substance classified with H360. Under the CLP group entry, lead compounds are in addition classified as chronically hazardous to the aquatic environment, category 1 (H410), as is lead chromate; for this property (HP 14) the annex multiplies the sum of such substances by 100 and compares it with 25 percent, so that by calculation a waste with a single lead compound is hazardous from as little as 0.25 percent by mass. Lead chromate is moreover classified as carcinogenic category 1B (H350) and thus falls under HP 7 from 0.1 percent by mass. For the eluate, the annex sets a separate limit for lead, 50 mg/kg dry matter (HP 15). A 0.03 percent value does not appear in Annex 3; the 0.03 percent sometimes cited comes from the CLP entry for metallic lead powder and from the German TRGS 505.

Two subtleties are decisive here. First, the values refer to the whole waste, not the coating layer alone: coated solid wood or metal dilutes the lead share, so the overall value usually lies well below the percentage of the pure coating. Pure stripping dust or flaked paint, by contrast, can exceed the thresholds. Second, waste law knows two ways of calculating: Annex 4 requires a measured result to be converted to the most probable compound ("auf die am wahrscheinlichsten zutreffende Verbindung umzurechnen"), but at the same time allows CLP Note 1 on calculation as metal to be taken into account "gegebenenfalls" (where appropriate; see the foldout above). In case of doubt, lead-containing removal material is treated as hazardous waste: if a hazard-relevant property cannot be ruled out, the ordinance assigns the waste to a hazardous waste type (Annex 2). It is handed over to a party authorised to collect or treat it (Waste Management Act 2002, section 15 paragraph 5).

Occupational safety: the most important part in practice

At the workplace it is not the resting coating that is the risk but working on it, and the values here have just been tightened considerably. In Austria an air limit for lead and its compounds of 0.03 mg/m³ as a daily average has applied since 31 December 2025 (short-term value 0.12 mg/m³, inhalable fraction, calculated as lead; Limit Value Ordinance as amended by BGBl. II No. 339/2025). Previously a MAK value (maximum workplace concentration) of 0.1 mg/m³ applied; it is now a TRK value (technical guidance concentration). The ordinance lists lead chromate not under lead but under the chromium(VI) compounds. For the assessment of fitness in the fitness and follow-up examinations, the Ordinance on Health Surveillance at the Workplace names a blood lead value of 30 µg/100 ml (i.e. µg/dl); its amendment (in force since 9 April 2026) limits this value to the end of 2028 and sets a value of 15 µg/100 ml from 2029. The basis is EU Directive 2024/869, which Austria has transposed with both ordinances.

There is also an application ban: paints and lacquers with a mass fraction of more than 2 percent lead may not be applied by spraying, except in closed apparatus (Limit Value Ordinance, section 27d paragraph 5). For particularly vulnerable groups, separate rules apply: expectant mothers may not be employed in work in which they are exposed to substances hazardous to health and harm cannot be ruled out (Maternity Protection Act, section 4 paragraphs 1 and 2 no. 4); for young people, work under exposure to reproductive toxicants is prohibited (KJBG Ordinance, section 3 paragraph 1 no. 1 lit. g), while young people in training may do it under supervision (section 3 paragraph 2). Lead is named explicitly in neither; for maternity protection it falls under the general rule, for young people via its classification.

In Germany, TRGS 505 "Lead" (February 2026 edition), as a recognised rule of technology, sets out the protective measures for activities with lead-containing mixtures from a lead content of 0.3 percent and, for powdery mixtures with a particle diameter below 1 mm, from 0.03 percent; the removal of lead-containing coatings is expressly within its scope, and its Annex 3 deals with the removal of lead-containing surface coatings on construction sites. Whether the dust produced when a coating is sanded itself falls under the 0.03 percent threshold as a powdery mixture, the TRGS does not say expressly. Read that way, the relevant threshold becomes ten times stricter on sanding: the resting coating is measured against the 0.3 percent mark, the fine sanding dust against the 0.03 percent mark.

For practice this means, regardless of the exact content: do not dry-sand, do not burn off, work with low dust, extract at source, wear respiratory protection.

Health: no safe value

The World Health Organization puts it plainly: there is no lead exposure known to be without harmful effects. Even blood lead levels from 3.5 µg/dl can be associated in children with reduced intelligence, behavioural problems and learning difficulties; the US health authority CDC lowered its reference value for children, which is based on the upper end of measured blood lead levels (97.5th percentile), from 5.0 to 3.5 µg/dl in 2021. Children absorb ingested lead up to four to five times as strongly as adults, and during pregnancy lead is released from the bone and reaches the unborn child (WHO). In adults, raised blood pressure, cardiovascular problems and kidney damage are to the fore (WHO).

Decisive for the real risk is the state of the coating: an intact, well-adhering coating is usually not a problem; it becomes critical with flaking paint, on friction surfaces such as windows and doors and in renovation work that disturbs the coating (US EPA); removal by blasting, burning, dry scraping, dry sanding and with power tools creates the most serious dangers (Australian environment department). The intermediate range is precisely where this distinction counts: intact and left alone, such a coating is usually unproblematic; if the German TRGS 505 is read as described under occupational safety, every one of the three example values lies, on sanding, many times above its 0.03 percent threshold for powdery mixtures.

All yardsticks compared

The following table places the limits side by side and sorts in the three constructed example values (0.2, 0.35 and 0.7 percent by mass). Important: material mass percent, area loading, air values and blood values are physically different quantities; only mass-based thresholds are directly comparable with a laboratory value in percent. Area values (mg/cm²) and air values appear in the table only for orientation.

Yardstick Threshold 0.2 % 0.35 % 0.7 %
New paint (US CPSC 16 CFR 1303; UNEP model law) 90 ppm (0.009 %) total lead above (~22x) above (~39x) above (~78x)
Dust value (DE TRGS 505, powdery mixtures <1 mm)* 0.03 % above (~7x) above (~12x) above (~23x)
CLP reproductive toxicity, mixture with lead compounds 0.3 % (as lead, Note 1) below above above
Existing "lead-based paint" USA (EPA/HUD) 0.5 % total lead (or 1.0 mg/cm²) below below above
Existing, Australia (AS/NZS 4361.2, according to Environmental Health Australia) 0.1 % by mass above above above
Waste hazardous (Waste Catalogue Ordinance 2020 Annex 3, in the whole waste) HP 10: 0.3 % of the H360 substance; HP 14: by calculation 0.25 % of a lead compound; HP 7 (lead chromate): 0.1 % depends on the substrate depends on the substrate depends on the substrate
"Lead paint" (building, AT and DE) no statutory threshold n/a n/a n/a
Workplace air when worked on 0.03 mg/m³ (air, not directly comparable) applies in dusty work applies in dusty work applies in dusty work

* TRGS 505 sets the 0.03 percent for powdery mixtures; whether the sanding dust of a coating falls under it, it does not say expressly (see occupational safety). The area-based values (US 1.0 mg/cm², France 1 mg/cm²) cannot be converted into a mass percentage and are therefore not entered column by column; the French laboratory value (1.5 mg/g, that is 0.15 percent) refers to acid-soluble lead and is not directly comparable with a total-lead value.

The reading in one sentence: all three values are unambiguously lead-containing and exceed the strictest new-paint yardstick many times over; but as "lead-based paint" under the US mass definition only the highest (0.7 %) qualifies; and the much-cited 0.3 percent mark, even where it is exceeded, does not mean what it is taken to mean: it remains a classification limit, not a lead-paint definition. And wherever the value lies exactly: lead becomes dangerous above all when the coating flakes, is abraded or is worked on and dust or chips are produced.

What this means in practice

A lead-containing old coating is no cause for panic and, as a rule, no remediation case as long as it is intact and left in peace. It is the working that becomes critical: sanding, burning off, breaking. Anyone renovating should not dry-sand lead-containing coatings and not burn them off, should work with low dust and, in case of doubt, treat the removal material as hazardous waste. Particularly important is protecting children and pregnant women from paint chips and house dust. And anyone wanting to know whether a particular coating contains lead at all, and how much, has it measured, on site with an X-ray fluorescence device or on a material sample in the laboratory; it cannot be judged with the naked eye.

Sources

  • CLP Regulation (EC) No 1272/2008, consolidated version of 1 July 2026: Annex I Table 3.7.2 (generic concentration limits for reproductive toxicity, 0.3 and 3.0 percent); Annex VI Part 1 section 1.1.3.2, Note 1 (concentration limits as percentages by weight of the metallic element); Annex VI Part 3: lead compounds (index 082-001-00-6; Repr. 1A, Aquatic Chronic 1; Note 1), lead chromate (082-004-00-2; Carc. 1B, Repr. 1A; Note 1), lead powder (082-013-00-1; specific limit 0.03 percent for H360D) and lead massive (082-014-00-7; no specific limit for reproductive toxicity): EUR-Lex 02008R1272. The two lead entries by particle size were introduced by Regulation (EU) 2016/1179 (recital 4; applicable from 1 March 2018): EUR-Lex 32016R1179.
  • Austrian Chemicals Prohibition Ordinance 2003 (Chemikalien-Verbotsverordnung), section 11d (lead carbonates and lead sulphates banned as constituents of paints): RIS. REACH Regulation (EC) No 1907/2006, consolidated version of 22 June 2026, Annex XVII, entries 16 (lead carbonates) and 17 (lead sulphates), ban as a paint constituent, and entry 30 with Appendix 5 (no supply to the general public): EUR-Lex 02006R1907.
  • US EPA, 40 CFR 745.103, definition of "lead-based paint" (at least 1.0 mg/cm² or at least 0.5 percent by mass): eCFR 40 CFR 745.103. Identically HUD, 24 CFR 35.86.
  • US CPSC, 16 CFR 1303.1, limit of 0.009 percent (90 ppm) for lead in consumer paint, calculated as metal, since 14 August 2009: eCFR 16 CFR 1303.1. UNEP, "Model Law and Guidance for Regulating Lead Paint" (2017, revised July 2018; developed with WHO and US EPA; 90 ppm total lead): UNEP. Canada, Surface Coating Materials Regulations (SOR/2016-193), section 2(1), 90 mg/kg: Justice Laws. Switzerland, ChemRRV (SR 814.81), Annex 2.8, 0.01 percent: Fedlex.
  • France, Arrêté of 19 August 2011 on the "constat de risque d'exposition au plomb", Article 5 (1 mg/cm² from X-ray fluorescence; with laboratory analysis 1.5 mg/g acid-soluble lead): Légifrance JORFTEXT000024524952. Australia, AS/NZS 4361.2:2017 (standard text paywalled); reduction from 1 to 0.1 percent by mass according to Environmental Health Australia (SA), "Technical Bulletin - Changes to AS/NZS 4361 Hazardous Paint Management": EHA SA. Australian environment department (DCCEEW), "Lead in house paint" (dangers of removal; as of April 2024): DCCEEW.
  • WHO and UNEP, "Update on the global status of legal limits for lead in paint" (March 2023): 93 countries with legally binding limits: WHO IRIS.
  • HUD, "Guidelines for the Evaluation and Control of Lead-Based Paint Hazards in Housing" (2012), Chapter 7 (inspection; XRF area loading, K and L X-rays, laboratory sample in percent by mass) and Appendix 1 (no conversion of mg/cm² to percent; on average 1 mg/cm² about 1 percent): Chapter 7, Appendix 1.
  • Waste Catalogue Ordinance 2020 (Abfallverzeichnisverordnung, BGBl. II No. 409/2020), Annex 2 (assignment in case of doubt), Annex 3 (HP 7 from 0.1 percent by mass of an H350 substance; HP 10 from 0.3 percent by mass of an H360 substance; HP 14 with the sum formula 100 × Σc(H410) ≥ 25 percent; HP 15 eluate lead 50 mg/kg dry matter) and Annex 4 (conversion to the most probable compound; Note 1): RIS, AVV Annex 3. Waste Management Act 2002 (AWG 2002), section 15 paragraph 5.
  • Limit Value Ordinance 2025 (Grenzwerteverordnung) as amended by BGBl. II No. 339/2025, Annex I/2025 (lead and its compounds excluding lead chromate, lead arsenate and lead chromate oxide: TRK 0.03 mg/m³ daily average, short-term value 0.12 mg/m³, inhalable fraction, calculated as lead; in force since 31 December 2025, section 35 paragraph 23); previously Annex I/2024 (BGBl. II No. 330/2024): MAK 0.1 mg/m³; section 27d paragraph 5 spray ban above 2 %: RIS, BGBl. II 339/2025. Ordinance on Health Surveillance at the Workplace (VGÜ), Annex 2 Part II point 1 lit. d (assessment: fitness): blood lead 30 µg/100 ml, limited to 31 December 2028 by BGBl. II No. 339/2025, Article 2 (in force since 9 April 2026); 15 µg/100 ml from 1 January 2029. EU Directive 2024/869 (transposed by Limit Value Ordinance section 33 and VGÜ section 11). Maternity Protection Act section 4 paragraphs 1 and 2 no. 4; KJBG Ordinance section 3 paragraph 1 no. 1 lit. g and paragraph 2.
  • TRGS 505 "Lead" (February 2026 edition, GMBl 2026 p. 146), section 1 (application from 0.3 and 0.03 percent lead content), Annex 3 (removal of lead-containing surface coatings; contents of up to several hundred grams per kilogram of paint): official state copy, Gewerbeaufsicht Baden-Württemberg.
  • WHO, "Lead poisoning" (no safe exposure value; blood lead from 3.5 µg/dl; children absorb up to 4 to 5 times as much; effects in adults): who.int. CDC, reference value 3.5 µg/dl (2021; 97.5th percentile): CDC MMWR 2021. US EPA, "Reduce the Risk of Lead Exposure at Home" (intact coating usually not a problem; friction surfaces; renovation): epa.gov.
  • Driers and lead pigments: Umiński, "Driers for Alkyd Coatings - an Overview", Paint & Coatings Industry, 1 September 2011: PCI. US Patent 4,631,087, "Surface coating compositions" (1986; conventionally 0.06 percent cobalt and 0.6 percent lead relative to the non-volatile medium): Google Patents. IARC Monographs Vol. 87, "Inorganic and Organic Lead Compounds" (2006, red lead as rust protection, lead chromate as yellow pigment); ColourLex, "Lead White": ColourLex.

Technical reference, not legal advice. Where else lead hides in old buildings, in pipes, dust and coatings, and the history behind it, is covered in our article on lead in the building.

Questions on the topic? → Contact

Let's talk about your building

Write to us or call.

Send a message

We'll get back to you within one business day.

Free

Direct line

The fastest way to reach us is usually in writing, by email. Prefer to talk your project through on the phone? Call us and we'll work out together which service fits and plan the next steps.

Free

Price calculator

Combine inspection, samples and travel and see the approximate cost immediately.

Estimate costs